How much does PLA shrink? Rate, Z and the value to enter

Printed PLA shrinks about 0.5% in X and Y and 0.8% in Z. Here are the figures by axis, the number each slicer's shrinkage field expects, and what PLA+ makers publish.

Written by 3D Calculators Team·Updated

The PLA shrinkage rate for printed parts is about 0.5% in X and Y and 0.8% in Z, so a 100 mm PLA (polylactic acid) part comes out roughly 99.5 mm long once it cools. Molded PLA resin shrinks 0.4%, according to NatureWorks.

How much does PLA shrink?

Printed PLA shrinks roughly 0.35 to 0.8%. In a Binghamton University study, PLA parts lost 0.63% in X, 0.35% in Y and 0.80% in Z. That averages about 0.5% across X and Y. NatureWorks lists 0.4% molding shrinkage for its Ingeo 3052D resin. Your own printer and settings will move these numbers.

Source Shrinkage Lost on 100 mm Lost on 25 mm
Printed PLA, X 0.63% 0.63 mm 0.16 mm
Printed PLA, Y 0.35% 0.35 mm 0.09 mm
Printed PLA, Z 0.80% 0.80 mm 0.20 mm
Molded PLA resin (no axis given) 0.4% ± 0.1% 0.40 mm 0.10 mm

The printed figures come from Weiser et al. (2021). They printed three part designs three times each in PLA on a QIDI X-One2 and measured them with digital calipers. That is nine PLA parts on one printer, so treat the figures as a starting point, not a constant. X and Y differed by almost half in that study, which is why a single XY number is a compromise.

The molded figure comes from NatureWorks’ sheet for Ingeo 3052D: 0.004 in/in, plus or minus 0.001. It describes melt packed into a steel mold under pressure. That says how the polymer behaves, but it gives no Z value and does not predict a printed part.

Does PLA shrink when it cools?

Yes. Bambu Lab’s wiki describes print shrinkage as thermal contraction: the plastic leaves the nozzle hot and contracts on its way down to room temperature, mostly in X and Y. Its test procedure says to measure only once the part has cooled to room temperature.

Whether 0.5% matters depends on the size. On a 20 mm part it is 0.1 mm. On a 200 mm part it is 1 mm, enough to stop a lid or a joint from fitting.

How much does PLA shrink after printing?

PLA shrinks about 0.5% in X and Y and 0.8% in Z after printing, all of it while the part cools to room temperature. From then on, its size changes for good only under heat, annealing or a steady load. Cold contracts it slightly, but the part grows back as it warms.

What acts on the part What happens Permanent?
Cooling to room temperature Shrinks 0.35 to 0.63% in X and Y, 0.80% in Z Yes, once
Cold: a -18 °C freezer, from a 20 °C room Contracts 0.16 to 0.38 mm per 100 mm No, it grows back when warm
Heat near the glass transition, 60 °C for Bambu Lab PLA Basic Can shrink and warp Yes
Annealing at 100 °C for 45 minutes (CNC Kitchen) Up to 10% smaller in X and Y, larger in Z Yes
A steady load (creep) Stretches slowly Yes

Heat is the change to plan for. Bambu Lab’s PLA Basic data sheet gives a glass transition of 60 °C and a heat deflection temperature of 57 °C under a 0.45 MPa load. Bambu Lab suggests annealing PLA Basic at 50 to 60 °C and warns that some prints deform and warp in the process. The guide to how PLA shrinks in heat has the figures for PLA, PETG and ABS and for parts left in a car.

Cold is reversible. SD3D and SUNLU list PLA’s thermal expansion at 41 and 101 millionths per °C, which gives the freezer row above: 100 mm x CTE x 38 °C = 0.16 to 0.38 mm. PLA in the cold works the numbers for a fridge, a winter garage and a fit on a metal shaft.

Creep stretches a loaded part slowly. Dogan (2022) loaded printed specimens of six materials for three hours at 25, 40 and 60 °C. PLA had the worst creep resistance, and the author recommends using PLA parts at room temperature with no load or only very low static loads.

What shrinkage compensation should you use for PLA?

Start with 0.49% in X and Y and 0.80% in Z, the averages from the Binghamton study. That means 99.51% and 99.20% in OrcaSlicer, 99.51% in Bambu Studio, 0.49% and 0.80% in PrusaSlicer, or a model scale of 100.49% and 100.81%. Then measure your own test part and replace them.

Where Field X and Y Z
OrcaSlicer Filament: Shrinkage (XY), Shrinkage (Z) 99.51% 99.20%
Bambu Studio Filament settings, Basic information: Shrinkage 99.51% no field; scale the object’s Z to 100.81%
PrusaSlicer Filament: Shrinkage compensation XY, Z 0.49% 0.80%
Any slicer’s scale tool Object scale 100.49% 100.81%

The fields expect different numbers:

  • OrcaSlicer and Bambu Studio want the cooled size as a percentage of the design. Their tooltip example is “94% if you measure 94mm instead of 100mm”. Both default to 100%, which means no compensation, and Bambu Studio’s field scales X and Y only.
  • PrusaSlicer wants the shrinkage itself: “if you measured 99mm instead of 100mm, enter 1%”. It defaults to 0%, accepts -10% to 10%, and shows the fields in Advanced and Expert mode.
  • Model scale wants the scale factor, 1 / (1 - shrinkage). For 0.49% that is 1 / 0.9951 = 1.0049, or 100.49%.

Use one method, not two. A shrinkage value in the filament profile plus a scaled model compensates the part twice.

How to account for PLA shrinkage on your own printer

  1. Calibrate flow first. Thin or fat walls shift every outside dimension by the same fixed distance, which is not shrinkage. The guide to dimensional accuracy calibration covers the order.
  2. Print a test part in the PLA you use, at least 100 mm long in X and Y and tall enough to measure Z. On 100 mm, 0.5% is 0.5 mm, easy to read with calipers.
  3. Let it reach room temperature, then measure each axis.
  4. Compute shrinkage as (designed - measured) / designed. A 100 mm side that measures 99.45 mm has shrunk 0.55%: enter 99.45% in OrcaSlicer or Bambu Studio, 0.55% in PrusaSlicer, or scale the model to 100.55%.

The shrinkage compensation calculator does that arithmetic for each axis and shows the value for each slicer field.

Does PLA+ shrink differently from regular PLA?

None of the PLA+ makers checked for this page publishes a figure showing it shrinks differently. Sunlu lists the same 0.1 to 0.3% for its PLA, PLA+ and PLA+ 2.0 and names no test method. The data sheets for eSUN PLA+, Overture PLA+ and PLA Pro, and Polymaker PolyLite PLA Pro give no shrinkage figure at all.

Filament Published shrinkage
Sunlu PLA, PLA+, PLA+ 2.0 0.1 to 0.3%, method not stated
eSUN PLA+ (data sheet V4.0, 2021) None
Overture PLA+ (V5.2) and PLA Pro (V5.1) None
Polymaker PolyLite PLA Pro None
Elegoo PLA+ None; the product page says only that it “minimizes warpage and shrinkage”

Sunlu’s range sits below both the printed-part figures (0.35 to 0.80%) and the molded resin figure (0.4%). Since Sunlu does not say how it was measured, do not enter it as a calibration value.

PLA+ and PLA Pro are not one material. Each maker modifies PLA its own way (eSUN describes its PLA+ as “modified based on PLA material”), so one brand’s result says nothing about another’s. Start PLA+ at the PLA values, then measure each brand with the steps above and save the result in that filament’s profile.

What PLA shrinkage compensation does not fix

  • Holes. Undersized holes come from polygon facets and extrusion width, not material shrinkage. Use the slicer’s X-Y hole compensation instead of scaling.
  • Annealing. Heat-treating PLA shrinks it far more than printing does. CNC Kitchen reported about 10% shrinkage in X and Y, with growth in Z. The calculator can stack an annealing step on top of print shrinkage.
  • Other filaments. In the same Binghamton study, PETG (polyethylene terephthalate glycol) shrank 0.54 to 0.76% in X and Y. ABS (acrylonitrile butadiene styrene) grew 0.92% in Z. A PLA value does not carry over to either.

Written by 3D Calculators Team· Published · Updated · Figures last checked

Sources

  1. Weiser et al., Shrinkage Compensation for FFF Printing for PLA, ABS, and PETG Thermoplastics (Binghamton University, 2021) (accessed 2026-10-13)
  2. NatureWorks, Ingeo Biopolymer 3052D technical data sheet, injection molding (archived copy) (accessed 2026-10-13)
  3. Bambu Lab Wiki, 3D prints shrinkage: causes and solutions (accessed 2026-10-13)
  4. OrcaSlicer Wiki, Material basic information (Shrinkage XY and Z) (accessed 2026-10-13)
  5. OrcaSlicer source, PrintConfig.cpp (filament_shrink and filament_shrinkage_compensation_z defaults and limits) (accessed 2026-10-13)
  6. OrcaSlicer Wiki, Precision settings (X-Y hole and contour compensation) (accessed 2026-10-13)
  7. Bambu Studio source, PrintConfig.cpp (filament_shrink) (accessed 2026-10-13)
  8. Bambu Studio source, fdm_filament_common.json (default filament_shrink) (accessed 2026-10-13)
  9. PrusaSlicer 2.9.2 source, PrintConfig.cpp (shrinkage compensation tooltips, defaults and limits) (accessed 2026-10-13)
  10. SUNLU Wiki, FDM filament performance comparison (accessed 2026-10-13)
  11. eSUN, PLA+ technical data sheet, Version 4.0, Nov. 2021 (archived copy) (accessed 2026-10-13)
  12. Overture, PLA+ technical data sheet, Version 5.2 (accessed 2026-10-13)
  13. Overture, PLA Professional technical data sheet, Version 5.1 (accessed 2026-10-13)
  14. Polymaker, PolyLite PLA Pro technical data sheet (accessed 2026-10-13)
  15. ELEGOO, PLA Plus 3D printer filament product page (accessed 2026-10-13)
  16. nophead, HydraRaptor blog: Polyholes (accessed 2026-10-13)
  17. CNC Kitchen, Annealing PLA prints: what it does and doesn't (accessed 2026-10-13)
  18. Bambu Lab, PLA Basic technical data sheet V3.0 (glass transition, heat deflection) (accessed 2026-11-08)
  19. SD3D, PLA technical data sheet (coefficient of thermal expansion; copy hosted by the Harvard SEAS 3D printing lab) (accessed 2026-11-08)
  20. SUNLU, PLA filament technical data sheet (coefficient of thermal expansion, ASTM E831; copy hosted by Electronilab) (accessed 2026-11-08)
  21. Dogan, Short-term creep behaviour of different polymers used in additive manufacturing under different thermal and loading conditions, Strojniški vestnik (Journal of Mechanical Engineering) 68 (2022) 451-460 (accessed 2026-11-08)

More from the blog

  • dimensional accuracy
  • shrinkage
  • flow rate

How to calibrate dimensional accuracy per material

Calibrate dimensional accuracy per material: fix e-steps and flow, print a test part, measure it, and turn the errors into XY, Z and hole compensation values.

  • dimensional accuracy
  • shrinkage
  • moisture

How to print dimensionally accurate nylon parts

Print dimensionally accurate nylon parts: dry the filament, control chamber and cooling, then compensate for print shrinkage and moisture swelling.