- dimensional accuracy
- shrinkage
- flow rate
Calibrate dimensional accuracy per material: fix e-steps and flow, print a test part, measure it, and turn the errors into XY, Z and hole compensation values.
- dimensional accuracy
- shrinkage
- moisture
Print dimensionally accurate nylon parts: dry the filament, control chamber and cooling, then compensate for print shrinkage and moisture swelling.
- shrinkage
- dimensional accuracy
Yes. 3D printed parts shrink as they cool, under 1% in X and Y for PLA, PETG and ABS. After that, only heat, moisture or a constant load changes their size.
- shrinkage
- dimensional accuracy
Yes. Printed PLA shrinks along its print lines and grows in height once it passes its glass transition, about 55 to 61 °C. Below that it barely moves.
- shrinkage
- dimensional accuracy
Yes, slightly and reversibly: a 100 mm PLA part loses 0.16 to 0.38 mm going from a 20 °C room to a -18 °C freezer. PETG loses about 0.19 mm.
- shrinkage
- dimensional accuracy
Printed PLA shrinks about 0.5% in X and Y and 0.8% in Z. The figures by axis, the molded resin value, and what to enter in OrcaSlicer, Bambu Studio and Prusa.
- slicer settings
- print time
- dimensional accuracy
Yes: thinner layers shrink the steps on curves and slopes, but 0.08 mm took 2.18 times as long as 0.20 mm in Bambu Lab's test. Filament use barely changes.
- scale
- dimensional accuracy
- filament weight
Yes, but walls under two lines (0.8 to 0.86 mm on a 0.4 mm nozzle), fine details and screw holes fail. At 200%, a solid part takes 8 times the plastic.
- tolerances
- dimensional accuracy
Counterbore hole 3D print sizes: for M3, model 6.5 mm wide and 3.4 mm deep over a 3.4 mm hole. Tables for M2 to M8 and #4 to 1/4 in, and printing it face down.
- tolerances
- dimensional accuracy
3D print countersink sizes: 90° for metric and 82° for inch flat head screws, 0.2 mm over the head's sharp diameter. M3 socket: 6.92 mm over a 3.4 mm hole.
- tolerances
- dimensional accuracy
A 3D print living hinge needs a web 0.4 to 0.6 mm thick, two or three layers. In a fold test, PP passed 1 million folds and PLA about 160. Sizes and settings.
- tolerances
- dimensional accuracy
3D print snap fit design: undercut = 0.67 × strain × length² ÷ thickness. Strain limits for PLA, PETG and ABS, 0.20 mm clearance per side, and print the arm flat.
- tolerances
- dimensional accuracy
How to 3D print hinges: a bore 0.40 mm over the pin for an assembled hinge, 0.30 to 0.40 mm per side printed in place. Sizes for filament, M3 and snap-on pins.
- tolerances
- dimensional accuracy
A 608 bearing is 8 mm bore, 22 mm outside and 7 mm wide. What 608ZZ and 608-2RS mean, and the hole to print: 21.90 mm press fit, 22.20 mm slip fit.
- tolerances
- dimensional accuracy
A 3D print annular snap fit needs an undercut of strain times diameter: about 0.5 mm on a 25 mm PLA cap and 0.9 mm in PETG, with the ring printed standing up.
- tolerances
- dimensional accuracy
3D print bearing press fit: draw the bore 0.10 mm under the bearing's outside diameter, 21.90 mm for a 608. Bore sizes for 623 to 6002, 6800, LM8UU and bushings.
- tolerances
- dimensional accuracy
D-shaft coupler or knob to 3D print: model 5.20 mm with 4.70 mm across the flat for a 5 mm stepper shaft. Bore sizes for 6 mm, 5 mm and 1/4 in D-shafts.
- tolerances
- dimensional accuracy
3D print magnet hole size: model the hole 0.10 to 0.15 mm over the magnet for a press fit, 0.20 to 0.30 mm for glue, and 0.1 to 0.2 mm deeper. Sizes by magnet.
- tolerances
- dimensional accuracy
3D print nut trap sizes for M2 to M8 and US nuts: model the hex pocket 0.2 mm wider than the nut across flats (5.7 mm for M3) and 0.1 mm deeper.
- tolerances
- dimensional accuracy
3D print O-ring groove sizes: make it 70 to 80% of the cross-section deep for 20 to 30% squeeze. Face and radial seal tables, a worked example and print settings.
- tolerances
- dimensional accuracy
3D print press fit tolerance: model 0.05 mm of interference per side (0.10 mm on the diameter) in PLA, less in ABS and nylon. Test print and pressing steps.
- tolerances
- dimensional accuracy
Print-in-place clearance: 0.30 to 0.40 mm per side in XY on a 0.4 mm nozzle and two whole layers in Z, with values for hinges, gears, toys and bearings.
- tolerances
- dimensional accuracy
3D print snap fit box lid sizes: a 1.35 mm skirt 0.20 to 0.25 mm per side inside the wall and a 0.3 to 0.5 mm catch, plus an ESP32 case and PCB clips.
- shrinkage
- dimensional accuracy
ABS shrinks about 0.4 to 0.8% in X and Y as it cools, but one printed-part study saw it grow 0.92% in Z. Figures by source, plus the OrcaSlicer values.
- shrinkage
- dimensional accuracy
ABS vs ASA shrinkage: about the same. Resin and filament data sheets put both at roughly 0.4 to 0.7%, so start ASA with ABS compensation and measure.
- shrinkage
- dimensional accuracy
Bambu Lab publishes no ABS shrinkage value. Start at 99.36% in Bambu Studio's Shrinkage field, then print a test cube and correct. PLA and PETG values too.
- shrinkage
- dimensional accuracy
PETG-CF shrinks about 0.3 to 0.6%, against 0.54 to 0.76% for printed plain PETG. The published PLA-CF and ABS-GF figures, and why X and Y can differ.
- shrinkage
- dimensional accuracy
Does PETG shrink? Yes, by under 1%: 0.54 to 0.76% in X and Y and 0.73% in Z in a printed-part study, close to PLA. Plus the value to enter in each slicer.
- shrinkage
- dimensional accuracy
Yes, 3D printed resin shrinks as it cures: 3 to 6% by volume on maker data sheets, and about 0.3 to 0.6% in X and Y on measured printed parts.